A flanged immersion heater bolts onto a tank nozzle. The elements weld into the flange. If a weld between tube and flange leaks, the tank drains out through the heater hole.
Weld type
Each tube gets a full penetration TIG weld around the flange hole. We use a backing bar so the root does not burn through. The weld must penetrate 100% - no cold lap, no incomplete fusion.
Materials
- Carbon steel flange (Q235): ER308L filler for stainless elements. The dissimilar weld handles the expansion difference.
- 304/316L flange: ER316L filler, match the base metal.
- Alloy 20 or Hastelloy: special filler, pre-heat 150 C to prevent cracking.
Pressure test
After welding, every flange goes on a test rack. We pressurize the water side to 1.5 times working pressure for 10 minutes. A 10 bar heater gets tested at 15 bar. We look at every tube-to-flange weld for weeping.
A customer's flange heater leaked hydraulic oil after 6 months. We found a pinhole in one tube weld that missed the pressure test (it was below the water line in our fixture). We redesigned the test rig to submerge the whole flange. Zero leaks in 3 years.
Weld appearance
A good TIG weld on stainless is shiny silver, no dark discoloration. Blue or black weld means the argon shield failed. That weld gets ground out and re-welded.
Need flanged heaters pressure-tested to your spec?
We test to 1.5x working pressure and provide a test report.
Send Your Specs