When you TIG weld a stainless tube end, the weld shrinks as it cools. That pulls on the tube and leaves residual stress. On long, thin heater elements, the tube bends like a bow. On high temperature service, the stress causes stress corrosion cracking.
What we do
After welding, we put the heater in an oven at 400 C for 1 to 2 hours. That lets the metal relax. The stress goes away. The tube stays straight when it cools.
When it matters
- Long elements over 1 meter - they bend without stress relief
- Austenitic stainless (304, 321) in chloride service - stress corrosion cracking
- Thick flange welds over 6 mm - high shrinkage stress
Small 100 mm cartridge heaters do not need it. The stress is small and the tube is short.
A customer received 1.5 meter finned tubular elements that were bent 10 mm from end to end. They would not fit in the oven duct. We added a stress relief cycle after welding. The tubes came out straight within 1 mm.
Need long straight elements?
We stress-relieve long elements. Straightness within 1 mm per meter.
Send Your Specs