Porosity is tiny gas pockets inside the weld. On a pressure vessel or immersion heater, one pinhole means a leak. We see it on about 2% of welds before we tightened the process.
Common causes
- Oil or grease on the tube end - cutting fluid from the saw. Clean with acetone before welding.
- Moisture on the filler wire - if the ER308L wire has been sitting in a damp shop, bake it at 150 C for 1 hour.
- Argon flow too low or too high - turbulent gas sucks in air. 8 to 12 L/min is the sweet spot.
- Draft in the weld shop - a fan blowing across the weld breaks the argon shield. Weld in a booth or shield with a drape.
What it looks like
A good TIG weld is flat and shiny. Porous welds look like orange peel - tiny bumps. X-ray shows black dots inside. On a water pressure test, bubbles come out of the pinhole.
We had a run of flange welds leaking. We traced it to a new shop assistant who used a dirty cloth to wipe the tube ends. The cloth had cutting oil on it. We now clean every end with a new acetone wipe right before welding. Porosity rate dropped to near zero.
Fixing porosity
Grind out the bad weld 100% to sound metal. Do not just weld over it - the gas pocket stays inside and leaks later. Reweld with clean parts and good gas.