Titanium sheath heaters go into seawater, chloride and acid tanks. Titanium resists corrosion that eats through stainless in weeks. But welding titanium is unforgiving.
The 400 C rule
Above 400 C, titanium reacts with oxygen, nitrogen and hydrogen in the air. The weld zone becomes brittle - like glass. It cracks on cooling. This is not just the weld pool - the heat affected zone (HAZ) on both sides also must be shielded.
How we weld it
- TIG welding with pure argon, 15 to 20 L/min
- Inside of tube purged with argon before and during welding
- Use a trailing gas cup that shields the hot weld as it cools below 400 C
- Color of a good Ti weld: silvery, like the base metal. Blue or gray means contamination, weld must be ground out.
Filler
ERTi-2 matching grade. No copper brushes, no steel tools - titanium must be welded with dedicated tools. Iron contamination on titanium causes rust spots in service.
A seawater filter press in Qingdao had titanium heaters failing in 4 months. We cut one open - the weld was blue and brittle. We welded new ones with full purge and trailing shield. They have run 4 years.
Need titanium heaters for chloride service?
We purge both sides and use dedicated Ti tools. Every weld is silver.
Send Your Specs