Inside every tubular heater, the nichrome resistance wire connects to the nickel lead wire. That joint is made by spot welding (resistance welding). It carries the full heater current.
Why spot weld, not twist
Twisted wire joints have high resistance. At 10A, that joint heats up more than the wire itself, oxidizes, and opens. A spot weld fuses the two metals into one - resistance near zero.
Parameters
- Electrode: copper alloy, water cooled
- Weld time: 0.05 to 0.2 seconds
- Current: 500 to 2000 A depending on wire gauge
- Force: just enough to hold the wires flat, not crush them
Testing the joint
After welding, we pull-test every joint. The wire should break outside the weld, not at the weld. If it breaks at the weld, the weld is cold and gets redone.
A batch of heaters failed in the field with open circuits. We cut them open - the nichrome had broken at the lead joint. The spot welder time had drifted to 0.02 seconds, making cold welds. We recalibrated and added a daily pull-test sample. No repeat failures.
Wire materials
Nichrome 80/20 connects to nickel lead wire (not copper). Copper would alloy with nichrome at high temp and become brittle. Nickel matches the expansion and stays ductile.
Need heaters with proven internal welds?
We spot weld every joint and pull-test samples daily.
Send Your Specs