Last year a customer in the Middle East sent us a photo: a 304 flanged heater that had been running on desalination brine for 8 months. The tubes were covered in pinholes. Water was leaking into the MgO, and the elements were shorting to ground. He wanted to know why the "stainless steel" heater failed.
Answer: 304 stainless is not all-purpose stainless. It's fine for clean water. It is not fine for chloride water. Here's what we tell every customer.
The number that matters: 200 ppm chloride
304 has no molybdenum. Above roughly 200 ppm of chloride in the fluid, it starts pitting — tiny corrosion holes that punch through the tube wall. The pits look small, but once they reach the resistance wire, the heater is dead.
316L has 2–2.5% molybdenum. It handles chloride levels up to several thousand ppm before pitting starts. That's why it's the standard for brine, seawater, swimming pools and coastal outdoor exposure.
When 304 is enough
Don't waste money on 316L if your application is any of these:
- Clean tap water, closed-loop water tanks
- Thermal oil, hot oil up to 300°C
- Dry air heating, ovens, duct heaters
- Platens, molds, press heating
- Food processing with water-based ingredients (not saltwater)
304 is cheaper, easier to bend, and readily available. For 9 out of 10 water heating jobs, 304 is the right call.
When you must go 316L
Switch to 316L (or higher) when:
- Seawater, brine, saltwater pools
- Any solution with chloride — bleach, fertilizer, pickling baths
- Outdoor coastal installations (salt in the air)
- Acid cleaning baths, sulfate or phosphate solutions
- Food-grade CIP systems with sanitizers that contain chlorine
- Operating temperature above 60°C with any chloride present (corrosion speeds up with heat)
When even 316L is not enough
We see this in plating and pickling lines. 316L won't survive hydrochloric acid, strong sulfuric, or sodium hypochlorite at high concentrations. In those cases, we switch to:
- Titanium — for seawater and acidic chloride solutions
- PTFE/PFA coated — for strong acids and aggressive chemicals
- Incoloy 800/840 — for high-temperature oxidation and sulfur atmospheres
We had a customer trying to heat 10% HCl with 316L tubes. They lasted 3 weeks. We replaced them with PTFE-coated elements and they've been running 4 years.
Why "L" matters
316L (low carbon, under 0.03%) is not the same as 316. The low carbon prevents carbide precipitation at the weld seam — which is exactly where intergranular corrosion starts. For any welded immersion heater, always specify 316L, not plain 316. The price difference is small, but the life difference is years.
Our rule: if the fluid spec sheet mentions "chloride," "salt," "brine" or "seawater," order 316L minimum. If it's just water or oil, 304 saves you money. If it's strong acid, don't even consider stainless — go PTFE or titanium.
Tell us what you're heating
Fluid type, concentration and temperature. We'll recommend 304, 316L, titanium or PTFE based on actual chemistry, not a guess.
Ask for Material Advice